【建筑(zhu)材料(liao)檢(jian)測方(fang)(fang)法(fa)】常用建筑(zhu)材料(liao)的檢(jian)測方(fang)(fang)法(fa) 建筑(zhu)材料(liao)取樣(yang)方(fang)(fang)法(fa)
建筑材料取樣方法
水泥
根(gen)據連續進場、等級、廠家、批(pi)號和品種都相同(tong)(tong)(tong)(tong)(tong)(tong)的(de)水泥(ni)(ni)作(zuo)為(wei)劃分依據,取(qu)(qu)樣(yang)(yang)單(dan)位(wei)同(tong)(tong)(tong)(tong)(tong)(tong)品種、同(tong)(tong)(tong)(tong)(tong)(tong)標號、同(tong)(tong)(tong)(tong)(tong)(tong)編(bian)(bian)(bian)號為(wei)一(yi)個(ge)取(qu)(qu)樣(yang)(yang)單(dan)位(wei),灌裝(zhuang)水泥(ni)(ni)應該(gai)進行分別編(bian)(bian)(bian)號和抽(chou)樣(yang)(yang),編(bian)(bian)(bian)號要按(an)照(zhao)水泥(ni)(ni)廠年生(sheng)產能力的(de)規(gui)定;每年10--30萬(wan)噸(dun)的(de)不得超過(guo)400t作(zuo)為(wei)一(yi)個(ge)編(bian)(bian)(bian)號;每年要是4--10萬(wan)噸(dun)的(de)不超過(guo)200t做為(wei)一(yi)編(bian)(bian)(bian)號。并且(qie)按(an)照(zhao)同(tong)(tong)(tong)(tong)(tong)(tong)一(yi)次進場的(de)有相同(tong)(tong)(tong)(tong)(tong)(tong)出廠編(bian)(bian)(bian)號的(de)水泥(ni)(ni)作(zuo)為(wei)一(yi)個(ge)取(qu)(qu)樣(yang)(yang)單(dan)位(wei),任意從至少3個(ge)相同(tong)(tong)(tong)(tong)(tong)(tong)罐車中取(qu)(qu)出同(tong)(tong)(tong)(tong)(tong)(tong)等量的(de)水泥(ni)(ni),經均(jun)勻混拌后取(qu)(qu)出至少12kg。另外,水泥(ni)(ni)存放保管也要符合相關要求。
鋼筋
鋼(gang)筋的(de)(de)取(qu)樣(yang)要按照同(tong)(tong)(tong)一牌(pai)號(hao)、爐罐號(hao)、規(gui)格(ge)、出廠日期和假貨狀態來進(jin)行劃分,一般(ban)情況下,一批鋼(gang)筋的(de)(de)重量不(bu)(bu)要大(da)(da)于60噸(dun)(dun)。其(qi)中冷拉鋼(gang)筋要進(jin)行分批驗收,一個檢驗批次(ci)應(ying)該是同(tong)(tong)(tong)直徑、同(tong)(tong)(tong)等(deng)級重量不(bu)(bu)大(da)(da)于20噸(dun)(dun)的(de)(de)冷拉鋼(gang)筋。另外對于重量在30噸(dun)(dun)以(yi)內的(de)(de)連續坯(pi)軋和冶煉(lian)爐鋼(gang)筋,可(ke)以(yi)使用(yong)同(tong)(tong)(tong)牌(pai)號(hao)、銅冶煉(lian)、同(tong)(tong)(tong)澆筑的(de)(de)方法(fa)混合成(cheng)批次(ci)進(jin)行,要注意的(de)(de)是每個批次(ci)不(bu)(bu)得(de)大(da)(da)于6個爐號(hao),并且每個爐號(hao)的(de)(de)含碳量相差不(bu)(bu)得(de)大(da)(da)于0.2%含錳量之差應(ying)該在0.15%以(yi)內。根據相關規(gui)定(ding),鋼(gang)筋取(qu)樣(yang)的(de)(de)流程(cheng)是:首先去掉(diao)鋼(gang)筋端頭500mm,然后再(zai)隨意截取(qu)鋼(gang)筋端頭500到(dao)1000mm,作為取(qu)樣(yang)。
建筑
木(mu)(mu)板(ban)取樣(yang)應該注意,同一(yi)(yi)品牌、品種、廠家、規格和類型的木(mu)(mu)板(ban)放在(zai)一(yi)(yi)個批次(ci),在(zai)實際(ji)的檢(jian)測工(gong)作(zuo)中我們通常(chang)是隨機按(an)照規定的面子截取一(yi)(yi)小塊木(mu)(mu)板(ban)作(zuo)為(wei)檢(jian)測樣(yang)品。
常用建筑材料的檢測方法
水泥
水泥的檢(jian)(jian)(jian)測(ce)主(zhu)要是(shi)對水泥的幾項(xiang)重(zhong)要指標進行相應的檢(jian)(jian)(jian)測(ce),主(zhu)要包括水泥細度的檢(jian)(jian)(jian)驗、水泥凝結時間檢(jian)(jian)(jian)測(ce)、水泥安定性檢(jian)(jian)(jian)測(ce)、水泥膠(jiao)砂強度檢(jian)(jian)(jian)測(ce)等。
1、水泥(ni)(ni)細(xi)度(du)(du)(du)檢(jian)(jian)測(ce)是根據(ju)《水泥(ni)(ni)細(xi)度(du)(du)(du)檢(jian)(jian)驗方法篩析法》(GB/1345―2005)。GB 175―2007規定(ding),評定(ding)水泥(ni)(ni)細(xi)度(du)(du)(du)是不是符合(he)標(biao)準要求(qiu),水泥(ni)(ni)細(xi)度(du)(du)(du)為選擇(ze)性指標(biao):礦(kuang)渣硅酸(suan)(suan)鹽(yan)水泥(ni)(ni)、火山灰質(zhi)硅酸(suan)(suan)鹽(yan)水泥(ni)(ni)、粉煤灰硅酸(suan)(suan)鹽(yan)水泥(ni)(ni)和(he)復(fu)合(he)硅酸(suan)(suan)鹽(yan)水泥(ni)(ni)的細(xi)度(du)(du)(du)都(dou)要要篩余(yu)表示,其80μm方孔(kong)篩篩余(yu)要小于(yu)10%或者(zhe)45μm方孔(kong)篩篩余(yu)不大于(yu)30%
2、水(shui)(shui)泥(ni)凝結(jie)時間(jian)(jian)檢(jian)測(ce)是根據《水(shui)(shui)泥(ni)標準稠(chou)度(du)、凝結(jie)時間(jian)(jian)、體(ti)積安定(ding)性檢(jian)測(ce)方法》(GB/T 1346―2001)和《通(tong)用(yong)硅(gui)(gui)酸(suan)鹽(yan)(yan)(yan)水(shui)(shui)泥(ni)》(GB 175―2007)的(de)規定(ding):硅(gui)(gui)酸(suan)鹽(yan)(yan)(yan)水(shui)(shui)泥(ni)的(de)首次(ci)凝結(jie)時間(jian)(jian)應該在45分(fen)(fen)鐘(zhong)以上,最終(zhong)凝結(jie)時間(jian)(jian)應該小(xiao)于390分(fen)(fen)鐘(zhong);普通(tong)硅(gui)(gui)酸(suan)鹽(yan)(yan)(yan)水(shui)(shui)泥(ni)、礦渣的(de)硅(gui)(gui)酸(suan)鹽(yan)(yan)(yan)水(shui)(shui)泥(ni)粉煤灰硅(gui)(gui)酸(suan)鹽(yan)(yan)(yan)水(shui)(shui)泥(ni)、火山灰質硅(gui)(gui)酸(suan)鹽(yan)(yan)(yan)水(shui)(shui)泥(ni)和復合硅(gui)(gui)酸(suan)鹽(yan)(yan)(yan)水(shui)(shui)泥(ni)的(de)初次(ci)凝結(jie)時間(jian)(jian)應該大于45分(fen)(fen)鐘(zhong),最終(zhong)凝結(jie)時間(jian)(jian)在600分(fen)(fen)鐘(zhong)以內。
3、水(shui)(shui)(shui)泥(ni)(ni)(ni)安定性檢驗(yan)依(yi)據《水(shui)(shui)(shui)泥(ni)(ni)(ni)標(biao)準稠度、凝結時(shi)間、體積安定性檢測方法》(GB/T 1346―2001)和《通(tong)用硅(gui)(gui)酸(suan)(suan)鹽水(shui)(shui)(shui)泥(ni)(ni)(ni)》(GB 175―2007)的規定,普通(tong)硅(gui)(gui)酸(suan)(suan)鹽水(shui)(shui)(shui)泥(ni)(ni)(ni)、硅(gui)(gui)酸(suan)(suan)水(shui)(shui)(shui)泥(ni)(ni)(ni)、礦渣硅(gui)(gui)酸(suan)(suan)鹽水(shui)(shui)(shui)泥(ni)(ni)(ni)、粉煤灰(hui)硅(gui)(gui)酸(suan)(suan)鹽水(shui)(shui)(shui)泥(ni)(ni)(ni)、火山灰(hui)質硅(gui)(gui)酸(suan)(suan)鹽水(shui)(shui)(shui)泥(ni)(ni)(ni)和復合硅(gui)(gui)酸(suan)(suan)鹽水(shui)(shui)(shui)泥(ni)(ni)(ni)安定性在沸(fei)煮法檢驗(yan)下必須達(da)到相關(guan)標(biao)準。
4、水(shui)(shui)泥膠砂強(qiang)度檢驗通過(guo)檢驗不同期(qi)間段的抗(kang)壓強(qiang)度、抗(kang)折強(qiang)度,來(lai)確定水(shui)(shui)泥強(qiang)度等級或(huo)者進行評(ping)定水(shui)(shui)泥強(qiang)度是不是和標準(zhun)要求(qiu)相(xiang)同。
鋼筋
在鋼(gang)(gang)筋(jin)(jin)(jin)(jin)進(jin)場(chang)時,首(shou)先檢(jian)查產品的(de)(de)(de)(de)合格證、出廠檢(jian)驗(yan)報告(gao)以(yi)(yi)及進(jin)場(chang)復驗(yan)報告(gao)等(deng)(deng)(deng)。鋼(gang)(gang)筋(jin)(jin)(jin)(jin)檢(jian)測的(de)(de)(de)(de)主(zhu)要項目包(bao)括:鋼(gang)(gang)筋(jin)(jin)(jin)(jin)的(de)(de)(de)(de)屈服強(qiang)度(du)、伸長(chang)率、抗拉(la)強(qiang)度(du)、焊接和沖擊檢(jian)驗(yan)、冷彎檢(jian)測以(yi)(yi)及反復彎曲(qu)等(deng)(deng)(deng)。鋼(gang)(gang)筋(jin)(jin)(jin)(jin)質量必須符合國家(jia)現行的(de)(de)(de)(de)標準GB13012《鋼(gang)(gang)筋(jin)(jin)(jin)(jin)混(hun)凝(ning)土用熱軋光圓(yuan)鋼(gang)(gang)筋(jin)(jin)(jin)(jin)》、GB1499《鋼(gang)(gang)筋(jin)(jin)(jin)(jin)混(hun)凝(ning)土用熱軋帶肋鋼(gang)(gang)筋(jin)(jin)(jin)(jin)》以(yi)(yi)及GB/T701《低(di)碳鋼(gang)(gang)熱軋圓(yuan)盤條》等(deng)(deng)(deng)規定和設(she)計要求。但是在現實的(de)(de)(de)(de)檢(jian)測過程中,有(you)些檢(jian)測人(ren)員不(bu)能夠嚴(yan)格地(di)執行國家(jia)檢(jian)測標準,比(bi)如光圓(yuan)鋼(gang)(gang)筋(jin)(jin)(jin)(jin)的(de)(de)(de)(de)力(li)學性能達(da)到了(le)Ⅱ級(ji)指(zhi)標,就判斷其(qi)實Ⅱ級(ji)鋼(gang)(gang),并(bing)且貿(mao)然按照Ⅱ級(ji)鋼(gang)(gang)筋(jin)(jin)(jin)(jin)來使用,實際上這些綱(gang)吉的(de)(de)(de)(de)屈服強(qiang)度(du)和抗拉(la)伸強(qiang)度(du)都低(di)于Ⅱ級(ji)鋼(gang)(gang)筋(jin)(jin)(jin)(jin)的(de)(de)(de)(de)十個百(bai)分點,如果在建筑(zhu)施工中,就相(xiang)當于比(bi)工程設(she)計圖(tu)少放了(le)10%的(de)(de)(de)(de)受(shou)力(li)鋼(gang)(gang)筋(jin)(jin)(jin)(jin),必然會影響建筑(zhu)工程的(de)(de)(de)(de)施工質量,對建筑(zhu)設(she)施造(zao)成安全隱患。
同時還應該注意,在對鋼(gang)(gang)筋(jin)進行(xing)檢測(ce)的(de)(de)過(guo)程中,應該采(cai)用(yong)(yong)鋼(gang)(gang)筋(jin)的(de)(de)公(gong)稱橫截(jie)(jie)面積對鋼(gang)(gang)筋(jin)強(qiang)度進行(xing)計(ji)算(suan),因(yin)為(wei)在建筑(zhu)市場上鋼(gang)(gang)筋(jin)的(de)(de)實(shi)際直接往往都(dou)小于公(gong)稱直徑,如(ru)果采(cai)用(yong)(yong)稱量法(fa)來(lai)計(ji)算(suan)其(qi)強(qiang)度值(zhi)的(de)(de)話,鋼(gang)(gang)筋(jin)試(shi)件會符合標準,但是再采(cai)用(yong)(yong)公(gong)稱截(jie)(jie)面積計(ji)算(suan)就不(bu)(bu)符合了(le),如(ru)果在建筑(zhu)施(shi)工中使用(yong)(yong)了(le)這些強(qiang)度計(ji)算(suan)錯誤的(de)(de)鋼(gang)(gang)筋(jin),那(nei)么必然會給建筑(zhu)施(shi)工結構帶來(lai)安(an)全隱(yin)患。同樣(yang)為(wei)了(le)保證試(shi)驗結果比較可信,也需要對檢測(ce)獲得的(de)(de)數據(ju)進行(xing)合理的(de)(de)修(xiu)約,比如(ru):按照《金屬材料室溫拉伸試(shi)驗方法(fa)》的(de)(de)規定,沒有具體要求的(de)(de)情況下,強(qiang)度值(zhi)大(da)于1000N/mm2時,修(xiu)約間(jian)隔應該為(wei)10N/mm2,強(qiang)度值(zhi)在200至(zhi)1000N/mm2時,修(xiu)約間(jian)隔應該為(wei)5N/mm2,當強(qiang)度值(zhi)不(bu)(bu)大(da)于200 N/mm2時,修(xiu)約間(jian)隔是1N/mm2。
木板
一般來講,人造板(ban)中(zhong)甲醛的(de)釋放量最(zui)主(zhu)要取(qu)(qu)決于其在生(sheng)產過程中(zhong)所使用的(de)膠黏劑(ji)、木(mu)材(cai)原料和環境(jing)等因素(su),具體的(de)檢(jian)測(ce)方法(fa)主(zhu)要有三種:靜態(tai)檢(jian)測(ce)法(fa)、動(dong)態(tai)檢(jian)測(ce)法(fa)和總量萃取(qu)(qu)法(fa)。
1、靜(jing)態檢測(ce)法,這(zhe)種(zhong)方(fang)法主要應用為干燥(zao)器法,具體(ti)的(de)(de)檢測(ce)步驟是(shi):把截(jie)取好的(de)(de)木板(ban)樣品(pin)放(fang)入存有(you)蒸(zheng)餾(liu)水的(de)(de)干燥(zao)器物中,使(shi)其在(zai)恒溫狀態下進行甲(jia)醛揮(hui)發,這(zhe)樣揮(hui)發出(chu)來(lai)的(de)(de)甲(jia)醛就會(hui)被(bei)底(di)部的(de)(de)蒸(zheng)餾(liu)水所溶解,然后(hou)計算木板(ban)樣品(pin)的(de)(de)面(mian)積和蒸(zheng)餾(liu)水中甲(jia)醛的(de)(de)含(han)量來(lai)得出(chu)甲(jia)醛的(de)(de)釋(shi)放(fang)量。
2、動態(tai)檢(jian)測(ce)法主(zhu)要是將待檢(jian)測(ce)的(de)(de)木(mu)板樣品(pin)放置在(zai)特定濕度、溫(wen)度、氣(qi)(qi)流量(liang)和壓力的(de)(de)氣(qi)(qi)候箱中(zhong),充(chong)分(fen)混(hun)合其(qi)釋放出的(de)(de)甲醛(quan)和載氣(qi)(qi),然后(hou)利用吸(xi)(xi)收(shou)瓶吸(xi)(xi)收(shou)氣(qi)(qi)候箱中(zhong)的(de)(de)氣(qi)(qi)體,然后(hou)測(ce)定出吸(xi)(xi)收(shou)液中(zhong)的(de)(de)甲醛(quan)含量(liang)、木(mu)板樣品(pin)表面積(ji)和吸(xi)(xi)收(shou)時間,計算(suan)出甲醛(quan)釋放量(liang)。
3、總量萃取(qu)法(fa)最(zui)常用(yong)的是穿(chuan)孔(kong)法(fa),適用(yong)于(yu)沒有經過飾面的擠壓刨花板、平壓刨花板和中密度纖維(wei)板。首先(xian),用(yong)沸騰的甲(jia)(jia)苯(ben)萃取(qu)所檢(jian)測(ce)的樣本中的甲(jia)(jia)醛(quan),然后將溶(rong)有甲(jia)(jia)醛(quan)的甲(jia)(jia)苯(ben)通過穿(chuan)孔(kong)器(qi)和水進行液(ye)液(ye)萃取(qu),讓甲(jia)(jia)醛(quan)溶(rong)于(yu)蒸餾水中,再(zai)驚醒(xing)測(ce)定(ding)。總量萃取(qu)法(fa)的過程不(bu)容易受(shou)到環(huan)境溫度的影響,所以其檢(jian)測(ce)結(jie)果(guo)較(jiao)好、數據較(jiao)可靠。但是萃取(qu)法(fa)所需的設備比較(jiao)復雜,操作(zuo)費用(yong)較(jiao)高,并且甲(jia)(jia)苯(ben)揮發(fa)對人體也是一種傷害,會造成(cheng)一定(ding)的污染。